①The main function of the cover rubber: protect the belt core, withstand the effects of abrasion, impact, cutting, corrosion and atmospheric environment caused by the conveyed materials, and meet the requirements of heat resistance, cold resistance, oil resistance, acid and alkali resistance, flame retardancy and static electricity. The characteristic requirements.
②From a technological point of view: the basic physical properties of the cover rubber have a great influence on the service life of the conveyor belt. The cover rubber compound needs to have better scorch resistance, calendering, extrusion and coating processing properties, and self-adhesive The surface should be smooth and bright after mutual adhesion, vulcanization or plasticization.
Design features of cover rubber:
①Selection of raw rubber:
1. Generally choose natural rubber to meet the requirements, because natural rubber has the best comprehensive performance, but also can choose styrene butadiene rubber, butadiene rubber, etc.
2. Generally, natural rubber is mainly used, and some styrene-butadiene rubber and butadiene rubber are mixed. On the one hand, it can reduce the cost, and on the other hand, it can also improve the process performance.
3. In order to ensure its strength requirements, higher elasticity and adhesion, the general glue content is 50-55%.
②Vulcanization system:
1. If all natural rubber is used, it is best to use sulfur as the vulcanizing agent, and the amount of sulfur is 2.5 parts.
2. If all styrene-butadiene rubber is used, the amount of sulfur is 2.0 parts, and if all butadiene rubber is used, the amount of sulfur is 1.2 parts.
3. If natural rubber and styrene butadiene rubber are used together at 50/50, the amount of sulfur is about 2.1 parts. If natural rubber and butadiene rubber are used together at 50/50, the amount of sulfur is about 1.6 parts.
4. As the amount of synthetic rubber increases, the amount of sulfur in the combined rubber is appropriately reduced, and the amount of accelerator is appropriately increased.
5. Generally, thiazoles are used as accelerators, and it is better to use M and DM together, because this can ensure a faster vulcanization speed and a longer scorch time.
6. Generally, zinc oxide and stearic acid are used as vulcanization activators, and the dosages are 5 parts and 2-3 parts respectively.
③Reinforcement filling system:
1. The reinforcing agent is mainly carbon black. Commonly used are high wear-resistant carbon black, semi-reinforcing carbon black, and general-purpose carbon black. The dosage is 40-50 parts.
2. In order to reduce costs, part of calcium carbonate, activated clay and other inorganic fillers can be added without affecting product performance.
④Softening system:
1. The elongation at break of the vulcanized covering rubber is about 500%, the hardness is 60-70 degrees (Shore A), the plasticity of the plasticized rubber is controlled at 0.25-0.30 (Wickers), and the rational use of softeners is for Improve the elasticity of the rubber and increase the process viscosity.
2. Pine tar oil is the best for NR, petroleum resin is better for SBR, and aromatic oil is better for butyl rubber. Generally, the amount of softener is 7-10 parts.
⑤Anti-aging system: The use conditions of the covering glue determine that it has certain requirements on the anti-aging performance. The chemical anti-aging agent generally uses amine anti-aging agent, the dosage is 1-2 parts, and the paraffin wax as the physical anti-aging agent is generally about 1 part.