Home > Knowledge > Content

Special performance requirements for heat-resistant and burn-resistant conveyor belts

Jan 12, 2022

①According to the different degree of heat resistance, it can be divided into different heat resistance grades, but all require no aging and cracking.

②Conveyor belts working in an environment with a temperature of 120°C:

a. Raw rubber: select mainly butadiene rubber and neoprene, with a rubber content of about 55%.

b. Vulcanization system: The raw rubber is mainly neoprene. The vulcanization system should choose 4 parts of magnesium oxide and 5 parts of zinc oxide. In order to speed up the vulcanization process and increase the tensile stress, 0.5-1.0 parts of thiazole accelerator NA can be added -22, but more than 1 part is easy to produce scorch.

The vulcanization system of styrene-butadiene rubber should adopt a low-sulfur and high-promoting vulcanization system.

c. Reinforcing agent: commonly used are high wear-resistant carbon black, etc., the dosage is 40-50 parts.

d. Softening system: mainly choose softeners with high boiling point and low volatility, commonly used are asphalt, motor oil, etc.

e. Anti-aging agent: Choose an anti-aging agent that has good heat resistance and aging resistance and is not easy to produce oil, such as MB, 10l, etc., and the dosage is 2-3 parts.

③Conveyor belt working under the temperature of 130℃:

a. Raw rubber: mainly butyl rubber, with a rubber content of about 50%.

b. Vulcanization system: Due to the low degree of unsaturation of butyl rubber and the difficulty of cross-linking, it can generally be cross-linked with resin, but it takes a long time and the efficiency is low. If sulfur is used for vulcanization, the amount of sulfur is 1.0 part, and the amount of accelerator should be appropriately larger, such as the amount of accelerator TT is 2.0 part, and the amount of DM is 1.0 part.

c. Reinforcing agent: Butyl rubber itself has high strength. Generally, high wear-resistant carbon black and semi-reinforcing carbon black can be used as the reinforcing agent, and the dosage is 40-50 parts.

d. Softener: Butyl rubber has low viscosity and only a little softener is needed. Generally, paraffin-based operating oil with high saturation is added.

e. Anti-aging agent: Due to the high saturation of butyl rubber and good resistance to heat and oxygen aging, it is generally not necessary to add anti-aging agent. If you have special requirements, you can add a small amount of anti-aging agent MB or RD, the amount is about 1 part.

④Conveyor belt working under 160-180℃ environment:

a. Raw rubber: EPDM rubber is generally used, with a rubber content of 50-55%.

b. Vulcanization system: Due to the high saturation of EPDM rubber, few double bonds, and slow sulfur cross-linking, it is advisable to use DCP (dicumyl peroxide) for cross-linking, and the dosage is 4-6 parts.

c. Reinforcing filler: generally add hard carbon black with good reinforcing property, the dosage is 40-50 parts.

d. Softener: It is best to use a softener with high boiling point and low volatility, such as anvil resin, and the amount is about 5 parts.

e. Anti-aging agent: Because the EPDM rubber has high saturation and good heat resistance and aging resistance, only a small amount of anti-aging agent, such as MB 1-2 parts, needs to be added.